What the numbers mean

Three numbering systems appear on almost every stainless steel enquiry, and confusing them causes most of the friction in a quotation.

  • AISI/SAE is the familiar trade number: 304, 316, 321, 310S. It is a designation, not a full specification.
  • UNS is the unified numbering system: S30400 for 304, S31603 for 316L, N08904 for 904L. It is precise and is what mill certificates normally quote.
  • EN 10088 is the European designation: 1.4301 for 304, 1.4404 for 316L, 1.4541 for 321, 1.4845 for 310S, 1.4539 for 904L.

All the grades discussed here are austenitic: face-centred-cubic structure, non-magnetic when annealed, and hardened by cold work rather than by heat treatment. That shared structure is why they look identical on the shelf and behave very differently in service.

The corrosion resistance comes from chromium. At roughly 10.5% and above, chromium forms a passive oxide layer a few nanometres thick that repairs itself in air or water. Nickel stabilises the austenitic structure and improves toughness; molybdenum improves resistance to pitting in chlorides; titanium and niobium prevent chromium carbide precipitation at temperature.

Comparison at a glance

Table 1 — Austenitic grades compared by typical composition and use
GradeUNSENCrNiMoTypical use
304 / 304LS30400 / S304031.4301 / 1.430718–20%8–10.5%—General fabrication, food contact, architecture
316LS316031.440416–18%10–14%2–3%Coastal, marine, chemical, pharmaceutical
321S321001.454117–19%9–12%—Welded parts in elevated-temperature service
310SS310081.484524–26%19–22%—Furnaces, kilns, high-temperature oxidation
904LN089041.453919–23%23–28%4–5%Sulphuric and phosphoric acid, severe chloride

304 and 304L

304 is the grade the industry defaults to, and for most indoor, food-contact and architectural work it is the correct answer. It combines 18% chromium with 8% nickel, withstands most organic chemicals and food acids, and is available in every form at the lowest cost of the austenitic family.

Its limits matter more than its strengths. 304 is not a marine grade: in coastal air it develops tea staining, and in splash zones it pits at inclusions and weld oxides. It is also not a high-temperature grade — above roughly 425 °C, chromium carbides form at grain boundaries, and the chromium-depleted zone beside them corrodes preferentially. That is called sensitisation.

304L (UNS S30403) caps carbon at 0.030% instead of 0.08%. Lower carbon leaves less carbide to form, so a weld in 304L retains more corrosion resistance than the same weld in 304. The base-metal corrosion resistance is essentially the same; the difference appears in the heat-affected zone.

If the part will be welded and cannot be solution-annealed afterwards, specify the L grade from the start. Upgrading after welding is not possible.

316L and the molybdenum effect

316L adds 2–3% molybdenum to the 18/8 base. Molybdenum raises resistance to pitting and crevice corrosion in chloride environments, which is why 316L is the minimum specification for coastal architecture, swimming pool structures, marine hardware and most chemical plant.

The practical test is the pitting resistance equivalent number, or PREN, calculated from chromium, molybdenum and nitrogen content. A 304 heat typically lands around 18–20; a 316L heat around 24–26. In chloride service, that difference is the difference between a surface that stays clean and one that pits within a couple of seasons.

316L is not a universal upgrade. It is softer than 304 in some cold-worked conditions, it costs more, and it still fails in warm, concentrated chlorides where a duplex or a 6% molybdenum grade is required. Use it where chlorides are present, not as a default.

321 and 347: stabilised grades

321 contains titanium at a minimum of five times the carbon content; 347 uses niobium plus tantalum. Both stabilisers combine with carbon at high temperature before chromium does, so the chromium stays in solution and the heat-affected zone does not sensitise.

That makes them the standard selection for exhaust systems, heat exchanger tube, furnace parts and refinery piping where service temperatures sit in the 425–815 °C band and post-weld annealing is impractical. Below that band they offer no advantage over 304L; above it, oxidation becomes the limiting mechanism and a higher-chromium grade takes over.

321 and 347 are usually interchangeable. The choice normally follows the project specification, or the product form and thickness that can be sourced in the required lead time.

310S: high temperature

310S carries 25% chromium and 20% nickel. That combination gives it resistance to oxidation and carburisation at temperatures where 304 and 316 would scale away, and it retains useful strength in continuous service up to roughly 1,000 °C depending on load and atmosphere.

The low-carbon "S" variant is specified for welded assemblies and for cyclic service. 310S is not a corrosion grade in the aqueous sense: it is not a better choice than 316L for seawater, and it is not a substitute for 904L in acid. It is a heat grade, and it is specified for furnace muffles, radiant tubes, kiln furniture and annealing fixtures.

904L: aggressive chemical service

904L (UNS N08904) is a super-austenitic grade with about 20% chromium, 25% nickel, 4.5% molybdenum and 1.5% copper. The copper addition is what makes it effective in sulphuric and phosphoric acid, where standard austenitics corrode rapidly.

It is also highly resistant to chloride pitting and stress corrosion cracking at moderate temperatures, which is why it appears in flue gas desulphurisation, fertiliser plant and acid transport. It is expensive and it work-hardens quickly, so it is specified deliberately rather than as insurance.

How to choose in four questions

  1. Is there chloride? Coastal air, sea water, de-icing salt, swimming pools, bleach or brine means 316L as a minimum. Warm concentrated chloride means duplex or 904L.
  2. Will it be welded and not annealed? Choose 304L or 316L instead of 304 or 316, or move to 321/347 if service temperature is above 425 °C.
  3. What is the service temperature? Below 425 °C, use the corrosion grade. Between 425 and 815 °C, use 321 or 347. Above 815 °C, use 310S or a heat-resistant cast grade.
  4. What is the chemical environment? Sulphuric or phosphoric acid points to 904L; nitric acid is usually handled by 304L; hydrochloric acid is a specialist problem that no standard austenitic solves.

Answer those four questions and the grade list usually narrows to one or two options. Send us the answers with the product form and quantity, and we will quote the grades that fit rather than the one that happens to be in stock.